title: "In-ditch examination and ILI verification"
description: "What the regulations require once the pipe is exposed: examine and look beyond the excavation, measure what the tool called, validate crack NDE for tight cracks, account for tool tolerance until it is verified, and feed the results back to the tool vendor."
section: assessment
updated: 2026-11-25
canonical: https://pipelinerepairs.com/assessment/in-ditch-examination/
markdown: https://pipelinerepairs.com/articles/assessment/in-ditch-examination.md
---

# In-ditch examination and ILI verification

In short. What the regulations require once the pipe is exposed: examine and look beyond the excavation, measure what the tool called, validate crack NDE for tight cracks, account for tool tolerance until it is verified, and feed the results back to the tool vendor.

An excavation is the one time an operator can measure the pipe directly. What is learned there has two uses: deciding what to do with the feature in the hole, and checking whether the inspection tool that sent the crew there can be trusted for the features nobody will dig.

## Examine, and look past the hole

[Section 192.459](https://www.ecfr.gov/current/title-49/section-192.459) requires that whenever any portion of a buried pipeline is exposed, the exposed portion be examined for evidence of external corrosion if the pipe is bare or the coating is deteriorated. If corrosion requiring remedial action under §§192.483 through 192.489 is found, the operator has to investigate circumferentially and longitudinally beyond the exposed portion, by visual examination, indirect methods, or both, to find additional corrosion that could need action. [Section 195.569](https://www.ecfr.gov/current/title-49/section-195.569) has the same structure for liquid lines. A dig for one ILI call that finds active corrosion at the edge of the bell hole is not finished at the edge of the bell hole.

## Measure what the tool called

**Metal loss.** Depth and length profiles by ultrasonic thickness, pit gauge, or laser scanning, referenced to a girth weld so the result can be matched to the tool call. The measured profile, not just the maximum depth, is what a profile method like RSTRENG needs. See the [worked comparison](/worked-examples/example-remaining-strength-methods/).

**Dents.** Depth and profile, location relative to welds, and whether there is metal loss, a gouge, or cracking in the dent. Each of those changes the regulatory bucket. See [Dents](/assessment/dents/).

**Cracks.** Surface methods (magnetic particle, often wet fluorescent) find and length-size surface-breaking cracks after coating removal and cleaning. Depth needs an ultrasonic method. [Section 192.714(g)](https://www.ecfr.gov/current/title-49/section-192.714) and the matching paragraph in §192.933 require that, whenever a gas transmission repair is required, known crack locations be directly examined with technology validated to detect tight cracks, those with a crack opening of 0.008 inch or less. The rule names inverse wave field extrapolation (IWEX), phased array UT (PAUT), and UT as examples. The procedures must have performance and evaluation standards, including surface cleanliness, confirmed by qualified subject-matter experts, and must account for sizing inaccuracy and fracture-model error.

**Hard spots.** On older pipe, PHMSA's 2024 [advisory on hard spots](https://www.federalregister.gov/documents/2024/11/18/2024-26725/pipeline-safety-identification-and-evaluation-of-potential-hard-spots-in-line-inspection-tools-and) warns that susceptibility from plate and pipe manufacturing is broader than earlier understood and could affect pipe made before 1970. It names coating degradation, soil chemistry, and increased hydrogen exposure as interacting threats that can lead to hydrogen-induced cracking. Field hardness testing at a dig is the usual way a hard-spot ILI call is confirmed or ruled out.

## Tool tolerance until verified

[Section 192.712(e)(1)](https://www.ecfr.gov/current/title-49/section-192.712) requires a gas operator to explicitly account for uncertainty in reported ILI results: tool tolerance, detection threshold, probability of detection and identification, sizing accuracy, interaction criteria, location accuracy, and unity plots or equivalent, unless the defect dimensions have been verified by in situ direct measurement. The practical effect is that a dig removes the tolerance for that feature, and a set of digs is how the operator shows the tool performed as specified for the rest.

A unity plot compares the tool's reported depth with the field-measured depth for every dig. If the points fall outside the tool's stated tolerance band more often than its confidence level allows, the tool specification cannot be relied on as stated. The operator then needs a larger tolerance, a re-analysis, or a re-run.

## Why the feedback loop matters

The Line 901 rupture in Santa Barbara County in 2015 is the public example. PHMSA's [ADB-2016-04](https://www.federalregister.gov/documents/2016/06/21/2016-14651/pipeline-safety-ineffective-protection-detection-and-mitigation-of-corrosion-resulting-from) reports that the last ILI run predicted external corrosion at the failure site with a maximum depth of 47% of wall. Post-failure laser scanning measured 89%. The bulletin also states that discrepancies between earlier ILI calls and the as-found sizes in correlation digs had not been shared with the ILI vendor to re-analyze the data. The NTSB's [Marshall report](https://www.ntsb.gov/investigations/AccidentReports/Reports/PAR1201.pdf) found a similar gap for cracks. The operator's engineering assessment used the crack depths reported by the 2005 ultrasonic crack tool without applying the tool's stated ±0.02-inch depth tolerance, without validating the reported wall thickness, and without considering interacting threats. The NTSB concluded that had the program included any of those, the defect that ruptured in 2010 might have been identified and addressed.

## The direct-assessment route

When external corrosion direct assessment (ECDA) is the assessment method rather than ILI, the dig is the third of four steps. Both parts incorporate NACE SP0502 for ECDA, and [§195.588](https://www.ecfr.gov/current/title-49/section-195.588) adds requirements such as at least two complementary indirect inspection tools per ECDA region. Direct examination results are used to validate the indirect survey, just as a dig validates an ILI run. For cased crossings, where ECDA is hardest, see [Cased crossings](/coatings/cased-crossings/).

## What the dig record should contain

- Feature ID and the tool's reported dimensions, alongside field-measured dimensions and the method used for each.
- The surface preparation done before NDE and the NDE procedure and technician qualification.
- Coating condition, soil and water observations, pipe-to-soil potential if measured.
- The extent of the circumferential and longitudinal investigation beyond the exposure.
- The decision, the repair if any, and the recoat. See [Coating at repair sites](/coatings/coating-at-repair-sites/).

## Sources

- [49 CFR 192.459, examination of buried pipeline when exposed](https://www.ecfr.gov/current/title-49/section-192.459) — eCFR
- [49 CFR 195.569, examination of exposed portions of buried pipelines](https://www.ecfr.gov/current/title-49/section-195.569) — eCFR
- [49 CFR 192.712(e), data and uncertainty](https://www.ecfr.gov/current/title-49/section-192.712) — eCFR
- [49 CFR 192.714(g), in situ direct examination of crack defects](https://www.ecfr.gov/current/title-49/section-192.714) — eCFR
- [49 CFR 195.588, direct assessment standards](https://www.ecfr.gov/current/title-49/section-195.588) — eCFR
- [ADB-2016-04, corrosion under insulated coatings (Line 901 ILI sizing discrepancy)](https://www.federalregister.gov/documents/2016/06/21/2016-14651/pipeline-safety-ineffective-protection-detection-and-mitigation-of-corrosion-resulting-from) — Federal Register
- [PHMSA advisory bulletin on hard spots and ILI, 89 FR 90827](https://www.federalregister.gov/documents/2024/11/18/2024-26725/pipeline-safety-identification-and-evaluation-of-potential-hard-spots-in-line-inspection-tools-and) — Federal Register
- [NTSB/PAR-12/01, Marshall, Michigan](https://www.ntsb.gov/investigations/AccidentReports/Reports/PAR1201.pdf) — NTSB