title: "Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)"
description: "Hydrostatic burst test of a pre-cured composite sleeve cut out after 25 years in gas service; pipe ruptured at 2,180 psi outside the repair."
section: case-studies
updated: 2026-11-25
canonical: https://pipelinerepairs.com/case-studies/cs-16-burst-test-of-a-composite-sleeve-repair-recovered-after-25-years-in-service-/
markdown: https://pipelinerepairs.com/articles/case-studies/cs-16-burst-test-of-a-composite-sleeve-repair-recovered-after-25-years-in-service-.md
---

# Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)

In short. Hydrostatic burst test of a pre-cured composite sleeve cut out after 25 years in gas service; pipe ruptured at 2,180 psi outside the repair.

Source: CSNRI, in World Pipelines (April 2021), describing a test on pipe removed by the operator (2020). Account type: Vendor field test.

In 1995 an operator repaired a 12-inch-long, 63-percent corrosion defect on a gas line (750 psi operating, 970 psi MAOP) with a pre-cured composite sleeve while the line stayed in service. At the end of 2020 that pipe section was cut out during other work and offered to CSNRI for testing. The repaired joint held 1,455 psi for five minutes and later burst at 2,180 psi, with the rupture in unrepaired pipe, not under the sleeve. Tensile tests on the old composite were reported at 90,000 psi. Because opportunities to test 25-year-old field repairs are rare, this is one of the more useful public composite data points, even though the write-up is by the manufacturer.

## Method

Clock Spring composite repair sleeve, originally installed in service over filler in corroded areas

## Defect

External corrosion, multiple defects; the worst was 12 inches long with 63 percent wall loss

## Pipe

Carbon-steel natural-gas pipeline operating at 750 psi, MAOP 970 psi, at the time of the 1995 repair. Diameter is not stated in the article.

## Outcome

The recovered, repaired joint was held at 1,455 psi (1.5 times MAOP) for five minutes, then taken to burst. It ruptured at 2,180 psi in pipe outside the repaired area. Coupon tensile tests on the 25-year-old composite were reported at 90,000 psi, which the authors say showed no meaningful degradation. The article is written by CSNRI, but it reports a full-scale test on a real field repair removed by the operator.

Schedule, cost, and service-life figures in this note are the publisher’s claims. They were not checked against an operator record or a laboratory report.

Dates: Repair installed in 1995. Pipe section removed and tested at the end of 2020. Article reprinted April 2021.

Maker named in the source: CSNRI (Clock Spring).

## Sources

- [Burst test of a Clock Spring repair recovered after 25 years in service (installed 1995)](https://www.cs-nri.com/wp-content/uploads/2021/05/CSNRI_AR_EN_World-Pipelines_April-2021.pdf) — CSNRI, in World Pipelines (April 2021), describing a test on pipe removed by the operator