title: "Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe"
description: "MFL-visible composite reinforcement of an internal weld defect on a 24-inch refined-products line cured at -7 C with heating blankets."
section: case-studies
updated: 2026-11-25
canonical: https://pipelinerepairs.com/case-studies/cs-18-weld-wrap-composite-reinforcement-of-an-internal-weld-defect-on-a-24-in/
markdown: https://pipelinerepairs.com/articles/case-studies/cs-18-weld-wrap-composite-reinforcement-of-an-internal-weld-defect-on-a-24-in.md
---

# Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe

In short. MFL-visible composite reinforcement of an internal weld defect on a 24-inch refined-products line cured at -7 C with heating blankets.

Source: WrapMaster / Tecma (vendor case-study PDF). Account type: Vendor account.

In-line inspection of a 24-inch Western European refined-products line (67 bar design) found a 12-by-15 mm internal weld defect, 5.1 mm deep. The regulator required reinforcement. The operator lowered pressure to 24 bar but kept the line full while trained technicians blasted the surface, applied epoxy, and installed a composite weld-wrap sleeve, which includes a metallic mesh so MFL tools can see the repair. Because the air temperature was -7 C, a heating blanket was used; the vendor says installation took less than an hour and the wrap was cured in four hours. This is a manufacturer PDF, but it gives unusually complete defect and pressure data.

## Method

WrapMaster Weld Wrap composite sleeve, designed to ISO 24817 and described as a permanent ASME B31.4 composite-sleeve repair, with a metallic mesh for MFL detectability

## Defect

Internal weld defect, 12 by 15 mm, 5.1 mm deep, found by in-line inspection

## Pipe

24-inch refined-products transmission pipeline, Western Europe, 67 bar gauge design pressure, 20 C operating temperature. Pressure was reduced to 24 bar gauge during installation and cure. Ambient temperature during installation was -7 C.

## Outcome

The vendor reports the sleeve was installed in less than an hour, fully cured within four hours under a heating blanket, and that the line stayed full of product at reduced pressure. Acceptance as a permanent repair is stated by the manufacturer with reference to ASME B31.4 and ISO 24817.

Schedule, cost, and service-life figures in this note are the publisher’s claims. They were not checked against an operator record or a laboratory report.

Dates: Year not stated. PDF hosted by a 2024-dated path.

Maker named in the source: WrapMaster.

## Sources

- [WrapMaster Weld Wrap reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe](https://tecma.it/wp-content/uploads/2024/04/WrapMaster-WeldWrap-24inch-Weld-Reinforcement-Tecma.pdf) — WrapMaster / Tecma (vendor case-study PDF)