# ASME B31G, Modified B31G, and RSTRENG

In short. What the three common remaining-strength methods actually assume, and which of them the federal rules name.

ASME B31G is the manual for the remaining strength of corroded pipe. It is the line-pipe method. API 579 is the broader fitness-for-service standard and is a different document. Three calculations travel under names that get swapped in spreadsheets. They are not the same.

**Original B31G** approximates the metal missing from a longitudinal profile as a parabola, two-thirds of the rectangle of maximum depth and length. Flow stress is 1.1 times SMYS. The Folias bulging factor is the two-term form √(1 + 0.8 L²/(Dt)), and the method uses it only while L²/(Dt) is 20 or less. Longer corrosion is treated with a remaining-wall equation, as if the patch were infinitely long. The PHMSA-hosted Kiefner paper on the Alliance Pipeline waiver describes those simplifications and notes that they made the method reliably conservative and, in places, more conservative than the failures justified.

**Modified B31G** keeps a single depth and length but changes three assumptions, as that paper and Kiefner and Vieth’s public development of the criterion describe them. Flow stress becomes SMYS + 10,000 psi. The missing area is taken as 0.85 times the rectangle, which is more conservative than a parabola as an area model and is usable on longer patches. The Folias factor returns to a closer approximation: √(1 + 0.6275z − 0.003375z²) for z = L²/(Dt) up to 50, and 3.3 + 0.032z beyond that. The [calculator](/assessment/calculators) implements these two closed forms and shows the switch.

**RSTRENG** (the effective-area method in PRCI report PR-3-805, also styled R-STRENG) does not assume 2/3 or 0.85. It steps along the measured depth profile, finds the combination of length and metal loss that governs, and applies the Folias factor to that effective area. It needs a river-bottom profile. A single maximum depth cannot run it. [Section 192.712(b)](https://www.ecfr.gov/current/title-49/section-192.712) names ASME/ANSI B31G and R-STRENG, and allows an alternative only when it is equally conservative, with prior notice to PHMSA if a less conservative method is proposed. [Section 195.452(h)](https://www.ecfr.gov/current/title-49/section-195.452) names B31G and PRCI PR-3-805 as suitable methods where a predicted burst pressure is compared with maximum operating pressure.

## What the methods are not for

They were built for blunt metal loss in ductile line pipe. A crack, a gouge with cold-worked metal at the root, and selective seam weld corrosion are fracture problems. Depth greater than 80 percent of the wall is outside the range in which the methods were meant to accept a defect; leak and measurement error dominate, and the gas and liquid integrity rules list metal loss greater than 80 percent of nominal wall as an immediate repair. The Kiefner paper’s caution, aimed at a pipeline seeking to operate at 80 percent of SMYS, is the right general warning: confirm the method still bounds the pipe you have before you lean on it for a high design factor or a high grade. SMYS + 10 ksi can sit close to the tensile strength of modern high-strength pipe.

The manual itself is copyrighted. The formulas on this site are the published engineering form of the criteria, cited to the public Kiefner sources and checked against the structure §192.712 requires. They are not a scan of the ASME tables. Use the incorporated edition when the regulation sends you there, and use a profile method when you have a profile.

## Sources

- [49 CFR 192.712 — Analysis of predicted failure pressure](https://www.ecfr.gov/current/title-49/section-192.712) — eCFR
- [49 CFR 195.452 — predicted burst pressure methods](https://www.ecfr.gov/current/title-49/section-195.452) — eCFR
- [Validity of standard defect-assessment methods (Kiefner & Associates, PHMSA-hosted)](https://www.phmsa.dot.gov/sites/phmsa.dot.gov/files/docs/technical-resources/pipeline/gas-transmission-integrity-management/65316/validityofcorrosionassessmentsr1.pdf) — PHMSA
- [Kiefner and Vieth, modified criterion, Oil & Gas Journal](https://www.ogj.com/home/article/17219618/evaluating-corroded-pipe-conclusion-pressure-calculation-for-corroded-pipe-developed) — Oil & Gas Journal
- [ASME B31G catalog entry](https://www.asme.org/codes-standards/find-codes-standards/b31g-manual-determining-remaining-strength-corroded-pipelines) — ASME