title: "In-service welding and hydrogen pipelines"
description: "Burn-through and hydrogen cracking when the line is still full, what API 1104 Annex B is for, and what changes when the product is hydrogen or a hydrogen-methane blend."
section: repair-methods
updated: 2026-11-25
canonical: https://pipelinerepairs.com/repair-methods/in-service-welding/
markdown: https://pipelinerepairs.com/articles/repair-methods/in-service-welding.md
---

# In-service welding and hydrogen pipelines

In short. Burn-through and hydrogen cracking when the line is still full, what API 1104 Annex B is for, and what changes when the product is hydrogen or a hydrogen-methane blend.

Welding on a line that still holds product is a different procedure from welding a pup in a shop. The steel under the arc is a pressure boundary, it is being cooled by whatever is flowing, and the weld has to be sound when the pressure comes back. Two ways that goes wrong have names: burn-through, and hydrogen cracking. A third, which shows up when the product is hydrogen or a hydrogen-rich blend, is hydrogen that enters the wall from the inside while the arc is on the outside.

API Standard 1104 is the pipeline welding standard. The in-service annex — Annex B in current editions, Appendix B in older ones — is where procedure qualification for welds made on pipe that contains product is set out. The annex is copyrighted and is not extracted here. What an operator takes from it, in substance, is a procedure qualified for the cooling rate the flowing line will actually produce, with the wall thickness, the heat input, and the hydrogen potential of the consumable under control. [Section 192.225](https://www.ecfr.gov/current/title-49/section-192.225) and [§195.214](https://www.ecfr.gov/current/title-49/section-195.214) already require a detailed, qualified procedure and a record of the qualifying tests. They do not spell out the annex. The procedure does.

## Burn-through

The puddle fails when the remaining ligament cannot hold the pressure at the temperature the arc has created. Thinner wall, higher pressure, and a process that dwells all push the same direction. The practical controls are the ones the repair tables already point at for weld deposition: the procedure states a minimum remaining thickness in the area to be welded and a maximum pressure during the repair, and the welder does not exceed either. Flow helps, because it carries heat off the inside surface, but flow is not a number in the procedure until someone has qualified at that flow. A fillet for a [Type B sleeve](/repair-methods/type-b-sleeves/) and a branch weld for a [hot tap](/repair-methods/hot-tap-and-plugging/) are the two places this shows up most often. A leak under the electrode is not a weld. It is product escaping into the arc.

## Hydrogen cracking

Hydrogen cracking is a delayed crack in a hard heat-affected zone. It needs hydrogen, a susceptible microstructure, and stress. Low-hydrogen consumables, preheat, and a cooling rate that does not leave a brittle zone are how procedures attack the three together. ASME B31.4’s notes on deposited weld metal require a low-hydrogen process. They do not define the hardness number. Public work on that number includes Bruce and Etheridge, IPC2012-90095, which is about heat-affected-zone hardness limits for in-service welds, on the [ASME Digital Collection](https://doi.org/10.1115/IPC2012-90095). A procedure copied from a shop weld on empty pipe will cool faster, or slower, than the same weld on a flowing line, and the hardness will not match the coupon. Qualify on a setup that reproduces the line.

Direct deposition of weld metal, which some codes allow for shallow external metal loss and for some gouges once the damaged metal is gone, is this problem in a small patch. It is not a general fill for a deep pit. The [selection note](/codes/repair-selection/) says which tables mark it limited.

## When the product is hydrogen

Natural gas and hydrogen are not the same welding problem. At ordinary operating conditions — pressures up to about 100 bar and metal temperatures up to about 60°C — commonly used low-alloy line pipe has been treated as not particularly susceptible to hydrogen embrittlement. That statement is about steady operation. It is not about a weld.

IPC2026-186302 measured absorption while welding on scaled hydrogen demonstrators, DN 50 to DN 300, walls about 4 to 7 mm, because a full-size weld on a pressurized hydrogen pipeline is rarely something a laboratory can do. More heat input, and a thinner wall, raised the temperature of the inside surface and the amount of hydrogen the steel took up. A double-pass weld held less hydrogen than a comparable single heavy pass. Oxide on vintage, corroded pipe behaved as a barrier: the old pipe absorbed less than bright machined pipe of the comparison set. After cooling, both the experiment and the diffusion model put the highest hydrogen between the weld metal and the heat-affected zone. The summary, and the limit that this is one set of demonstrators, is in the [research library](/research/library/).

A companion public discussion is Bruce, Boring, Gould, and Huising, “In-Service Welding onto Hydrogen and Methane/Hydrogen Mixture Pipelines,” PRCI-EFS2023-029, at the 2023 Emerging Fuels Symposium. It is not a federal rule. PHMSA’s research program is the public index for what the agency has sponsored on emerging fuels; it does not, by itself, approve a welding procedure.

Blends change the partial pressure of hydrogen, which is the driving force for absorption, not the name on the tariff. A procedure qualified on methane is not a procedure qualified on hydrogen until the hydrogen case has been run. The same is true in the other direction: a result on pure hydrogen is not automatically the result on a 10 percent blend, or on a 90 percent blend.

## What this does not authorize

Nothing here is a heat input, a preheat, or an electrode classification. Those live in the qualified procedure. A [compression sleeve](/repair-methods/compression-sleeves/) avoids welding to the carrier, which is one reason it is discussed for laminations and for in-service pipe where a fillet on the pressure boundary is the risk being avoided. The long seams of that sleeve are still welds, made to the operator’s procedure, and they are not welds on the live wall only if the arc stays off that wall. A sleeve that must be welded to the carrier on a hydrogen line is the IPC2026-186302 problem, not the compression-sleeve problem.

## Sources

- [API Standard 1104, Welding of Pipelines and Related Facilities](https://www.api.org/products-and-services/standards/important-standards-announcements/1104) — API
- [Bruce and Etheridge, IPC2012-90095, heat-affected zone hardness limits](https://doi.org/10.1115/IPC2012-90095) — ASME
- [Erxleben and others, IPC2026-186302, hydrogen absorption during in-service welding](https://asmedigitalcollection.asme.org/IPC) — ASME
- [49 CFR 192.225, welding procedures](https://www.ecfr.gov/current/title-49/section-192.225) — eCFR
- [49 CFR 195.214, welding procedures](https://www.ecfr.gov/current/title-49/section-195.214) — eCFR
- [PHMSA pipeline research](https://primis.phmsa.dot.gov/rd/) — PHMSA