title: "Fatigue and burst testing of composite and steel-sleeve repairs on corrosion and dents, 2014"
description: "On 75 percent corrosion, a composite repair leaked at 198,550 cycles and Type A and Type B sleeves reached a 302,465-cycle run-out. On 15 percent dents, the composite repair failed at 149,913 cycles and the sleeves reached 239,897 cycles without failure. All three corrosion burst samples failed in base pipe outside the repair, at 4,480, 4,233, and 4,290 psi."
section: test-reports
updated: 2026-11-25
canonical: https://pipelinerepairs.com/test-reports/composite-and-steel-sleeve-repairs-corrosion-dents-2014/
markdown: https://pipelinerepairs.com/articles/test-reports/composite-and-steel-sleeve-repairs-corrosion-dents-2014.md
---

# Fatigue and burst testing of composite and steel-sleeve repairs on corrosion and dents, 2014

In short. On 75 percent corrosion, a composite repair leaked at 198,550 cycles and Type A and Type B sleeves reached a 302,465-cycle run-out. On 15 percent dents, the composite repair failed at 149,913 cycles and the sleeves reached 239,897 cycles without failure. All three corrosion burst samples failed in base pipe outside the repair, at 4,480, 4,233, and 4,290 psi.

Source: Alexander, C., and Vyvial, B. (Stress Engineering Services, Inc.), and Wilson, F. (Armor Plate, Inc.). “Pipeline Repair of Corrosion and Dents: A Comparison of Composite Repairs and Steel Sleeves.” Proceedings of the 10th International Pipeline Conference, paper IPC2014-33410, Calgary, Alberta, 29 September–3 October 2014. ASME. DOI: [10.1115/IPC2014-33410](https://doi.org/10.1115/IPC2014-33410).

## What was tested

One composite repair system (Armor Plate Pipe Wrap), a Type A steel sleeve, and a Type B steel sleeve, used to repair machined 75 percent corrosion and 15 percent plain dents. Burst tests were run on the corrosion samples. Fatigue tests were run on both the corrosion and the dent samples.

## Setup

Corrosion samples were 12.75-inch outside diameter, 0.375-inch wall, Grade X42 (SMYS pressure 2,470 psi; MAOP 1,780 psi at 72 percent of SMYS). Dent samples were 12.75-inch outside diameter, 0.188-inch wall, Grade X42 (SMYS pressure 1,239 psi; MAOP 890 psi). An incompressible putty-type filler was used in the corrosion and dent regions. Three 15 percent dents were installed in each dent sample with a 4-inch spherical end cap, with the pipe at 72 percent of SMYS (890 psi) during indentation, followed by ten cycles from 0 to 890 psi. The composite thickness on the dent samples was 0.313 inch (five layers, 1.5 times the 0.188-inch wall), from design calculations made before the repair. Corrosion fatigue samples were cycled from 890 to 1,780 psi (a 36 percent SMYS range). Dent fatigue samples were cycled from 100 to 990 psi (a 72 percent SMYS range). Burst samples were held at 1,780 psi and at 2,470 psi, then taken to failure.

## Key numbers

Burst of the 75 percent corrosion samples. All three failed in the base pipe outside the repair: 4,480 psi for the composite repair, 4,233 psi for the Type A sleeve, and 4,290 psi for the Type B sleeve. Hoop strain in the steel at the center of the repair, at 72 percent of SMYS, was 2,191 microstrain under the composite, 1,919 microstrain under the Type A sleeve, and 2,153 microstrain under the Type B sleeve. The paper notes that those three strains are within 15 percent of one another.

Fatigue of the 75 percent corrosion samples. The composite repair leaked in the corrosion area after 198,550 cycles. Neither steel sleeve failed; cycling was stopped at 302,465 cycles after the run-out target was passed.

Fatigue of the 15 percent dent samples. The composite repair failed in a dent after 149,913 cycles. Both steel sleeves reached 239,897 cycles without failure, after which cycling was stopped.

The paper also converts those lives, with a fatigue safety factor of 10 and a “moderately aggressive” gas-pipeline spectrum (337 cycles per year at 36 percent of SMYS; 25 cycles per year at 72 percent of SMYS), to 58 years for the composite corrosion repair and at least 90 years for the sleeves, and to 594 years and 952 years for the dent repairs. Those years are the paper’s arithmetic. The sleeve figures are lower bounds, because those samples did not fail.

## Takeaways

On these samples, burst of the 75 percent corrosion repairs occurred in the carrier pipe outside the repair, at similar pressures, and the hoop strain under the composite at 72 percent of SMYS was close to the strain under the two sleeves. In pressure cycling, the Type A and Type B sleeves were taken past the composite repair’s failure without a sleeve failure, on both the corrosion and the dent matrices. The cycle counts for the sleeves are run-outs, not measured lives to failure.

The paper is available from [ASME](https://doi.org/10.1115/IPC2014-33410).

## Sources

- [Pipeline Repair of Corrosion and Dents: A Comparison of Composite Repairs and Steel Sleeves (IPC2014-33410)](https://doi.org/10.1115/IPC2014-33410) — ASME 10th International Pipeline Conference, 2014