# Steel sleeves reinforcing corrosion and plain dents, 2021

In short. Type B sleeves on 24-inch corrosion and dent samples raised the equivalent fatigue life relative to bare pipe. The report’s highlighted lives are its own conversion.

Source: Allan Edwards, Inc.; testing by ADV Integrity, Inc. (2021). Project AE-17-006, updated November 2021. Dr. Chris Alexander, PE. Running headers in the body still show 20 January 2019; the update adds 2021 re-tests, including sample 24D-AESS-306.

## What was tested

Six Type B samples: three with machined corrosion, 12 inches by 6 inches and 50 percent deep, on 24-inch by 0.375-inch Grade X65 pipe, and three with plain dents on 24-inch by 0.250-inch Grade X52 pipe dented at 50 percent of SMYS. One corrosion sample and one dent sample were left bare.

## Setup

Reinforced samples were cycled 50,000 times. A hole was then drilled to simulate a through-wall leak, and cycling continued, typically until a sleeve-weld leak. Cycles were converted with Miner’s rule to an equivalent range of 72 percent of SMYS. Design life in the report uses a safety factor of 5 and a “light” cycling spectrum from Kiefner and others, IPC2004-0167.

## Key numbers

Under that light spectrum the report lists 5,336 cycles and 106 years for unreinforced corrosion, against 21,247 cycles and 424 years and 32,020 cycles and 640 years for the reinforced corrosion sleeves, about 4 and 6 times the bare life. Unreinforced dents lasted 13,004 cycles and 260 years, against 29,743 and 594 years, 30,391 and 607 years, and a mid-2021 fit-up re-test (24D-AESS-306) of 42,551 cycles and 851 years. Reinforced corrosion hoop-strain ranges were about half the bare sample. Reinforced dent hoop strains were 22 to 28 percent of the bare sample.

## Takeaways

The calendar years are the report’s arithmetic for a lightly cycled gas line, not a federal design life. The report says that without the drilled holes a failure before 100,000 cycles was considered unlikely, and that filler and fit-up changed the result. No composite results are in this report.

[Download the report](/downloads/updated-sleeves-test-program-2021.pdf).

## Sources

- [Steel sleeves reinforcing corrosion and plain dents, 2021](/downloads/updated-sleeves-test-program-2021.pdf) — Allan Edwards / ADV Integrity