title: "Type B sleeve fit-up, tight and loose, 2021"
description: "On 24-inch pipe with a through-hole, a tight Type B sleeve leaked after 4,934 cycles and a loose sleeve after 1,382."
section: test-reports
updated: 2026-11-25
canonical: https://pipelinerepairs.com/test-reports/steel-sleeve-fit-up-2021/
markdown: https://pipelinerepairs.com/articles/test-reports/steel-sleeve-fit-up-2021.md
---

# Type B sleeve fit-up, tight and loose, 2021

In short. On 24-inch pipe with a through-hole, a tight Type B sleeve leaked after 4,934 cycles and a loose sleeve after 1,382.

Source: Allan Edwards, Inc.; testing by ADV Integrity, Inc. (2021). Report 100160-RP01-Rev2-022521, February 2021. Letter signed by Dr. Chris Alexander, PE.

## What was tested

Two Allan Edwards Type B sleeves, 24-inch outside diameter by 0.375-inch wall, ASTM A572 Grade 65, one a tight fit and one a loose fit.

## Setup

Each sleeve was installed on 24-inch outside diameter, 0.25-inch wall, Grade X52 pipe with a 1/2-inch through-hole, so the sleeve was pressure-containing. Both were cycled from 100 to 867 psig, about 9 to 80 percent of SMYS.

## Key numbers

The tight sleeve leaked in the long-seam weld after 4,934 cycles. The loose sleeve failed the same way after 1,382 cycles, 3,552 cycles sooner.

## Takeaways

On this pair, a looser fit used up the seam weld much earlier. The report treats fit as the variable that keeps stress down in the carrier and in the sleeve welds. It does not compare a second manufacturer.

[Download the report](/downloads/steel-sleeve-fit-up-test-program-2021.pdf).

## Sources

- [Type B sleeve fit-up, tight and loose, 2021](/downloads/steel-sleeve-fit-up-test-program-2021.pdf) — Allan Edwards / ADV Integrity