05 · Defect assessment

Screening calculators

Hoop stress, code design pressure, and the two closed-form corroded-pipe criteria. The arithmetic runs in your browser. Nothing is uploaded.

Hoop stress and design pressure

Hoop stress uses Barlow’s thin-wall formula, σh = PD / (2t), with nominal outside diameter and nominal wall, which is the geometry in §192.105. Gas design pressure is P = (2St/D) × F × E × T. Hazardous-liquid internal design pressure under §195.106 drops the temperature factor. Neither result is MAOP or MOP. Tabulated sleeve-wall pressures, with the same Barlow form, are on the steel repair sleeve MAOP tables.

Units

Do not add extra thickness that was provided only for external loads. See §192.105(a).

Class-location factors have exceptions for stations, fabricated assemblies, and offshore pipe. Read the section.

Seamless and modern welded line pipe are often 1.00. Confirm the seam against the table in §192.113.

Section 192.115 says to interpolate between tabulated temperatures. Section 195.106 does not use T; it is ignored for the liquid formula.

Result

Enter the pipe data, or load the worked example: 24 in × 0.375 in, X52, 1,000 psig, Class 1 factors. Design pressure for that case is 1,170 psig. Hoop stress at 1,000 psig is 32,000 psi, about 61.5 percent of SMYS.

B31G and Modified B31G

Both methods estimate the pressure at which a blunt, axially oriented metal-loss patch fails in ductile line pipe. Original B31G uses a parabolic area (2/3), flow stress of 1.1 × SMYS, and a two-term Folias factor, switching to a remaining-wall equation when L²/(Dt) exceeds 20. Modified B31G uses an area factor of 0.85, flow stress of SMYS + 10,000 psi, and a three-term Folias factor. RSTRENG, which integrates a depth profile, is named in §192.712 and is not computed here. Read the B31G note before treating a number as an acceptance.

Units

Deepest point of a blunt corrosion patch. Not a crack depth, and not a gouge.

Length along the pipe axis. Circumferential width is not an input to these two formulas.

Used only to divide the predicted failure pressure. It does not check class location, HCA status, or tool tolerance.

Result

Enter a corrosion patch, or load the worked example: 24 in × 0.375 in, 52,000 psi SMYS, 0.150 in deep by 6 in long, compared with 1,000 psig. For that case the original criterion returns about 1,507 psig and the modified criterion about 1,565 psig.