05 · Defect assessment
Gouges and mechanical damage
In short Why a gouge is not metal loss, how grinding and the liquid-line 12.5 percent criterion fit together, and what must not be left under a sleeve.
A gouge is metal removed by contact. Excavator tooth, sled, rock, a chain. The groove is sharper than corrosion, the metal at the root is often torn and cold-worked, and cracks start there without announcing themselves as “crack-like” on the first visual pass. Calling the depth a corrosion depth and running B31G on it treats a notch as a blunt patch. Section 192.712 sends mechanical damage that can create a stress riser down the dent-and-mechanical-damage paragraph, not automatically down the corrosion paragraph.
PHMSA’s fact sheet describes grinding as a repair when it eliminates the concentrating effect and does not take so much wall that the pressure capacity is gone. The sequence that matches both the fact sheet and the dent research is: clean, inspect for cracks with magnetic particle or dye penetrant, grind to sound metal, inspect again, measure what remains, then decide. The decision is accept and recoat, reinforce, or cut out. Many operators forbid the “accept” branch. The fact sheet says that is common. A remaining-wall calculation after a successful grind is a metal-loss calculation on a smooth dish. A calculation before the cracks are gone is not.
On liquid integrity-management segments, a gouge or groove deeper than 12.5 percent of nominal wall is a 180-day condition under §195.452(h), unless a stricter immediate or 60-day criterion also applies. The July 2026 proposal says PHMSA is not proposing to change that gouge-or-groove criterion. Even as a proposal, that sentence is a signal: the 12.5 percent trigger is not an antique the agency has already walked away from. It is also not the only trigger. A gouge on the top of the pipe inside a dent is an interacting feature, and both the gas immediate-dent criterion and the liquid dent criteria are written for that combination.
What does not count as a repair
Leaving the gouge under a composite wrap or a Type A sleeve, because the sleeve “carries the load,” is the practice public enforcement has treated as a failure to follow procedures that required the defect to be ground out. The stress concentrator is still in the steel. Cyclic pressure finds it. The composite note and the Type A note are the method pages. The rule on this page is the order of operations.
A gouge that has torn into a longitudinal or girth weld is a weld repair. Grinding a weld without a procedure qualified for that weld is how a shallow scrape becomes an unrepaired seam defect with a shiny surface. When the remaining ligament after an honest grind is below what §192.485 or §195.585 allows, the grind was preparation for a cut-out or a designed reinforcement, not the repair itself. Recoat either way. Bare grind marks corrode into pits, and the next ILI run will call them metal loss that nobody can tie back to the excavation.
Sources
- PHMSA fact sheet: Pipeline repairs, grinding — PHMSA
- 49 CFR 195.452(h) gouge criterion — eCFR
- 49 CFR 192.712 — eCFR
- TTO-10 dent study — PHMSA
- 2026 NPRM, gouges as an interacting dent threat — Federal Register
Related notes
- Grinding and recoat — Repair methods
- Part 195 repair and integrity duties — Regulations and official guidance
- ASME B31.4 — Codes and standards
- Type B steel sleeves — Repair methods
Also in Defect assessment
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction