05 · Defect assessment
Vintage LF-ERW seams
In short Why pre-1970 low-frequency electric-resistance-welded seams are a longitudinal-seam threat, how that differs from modern high-frequency ERW, and what an assessment has to be able to see.
Low-frequency electric-resistance-welded pipe made before about 1970 is a longitudinal-seam problem, not a body-wall corrosion problem that happens to sit near a weld. The bond was made with low-frequency alternating current. The heat-affected zone is wide. The defects that show up in that seam — cold welds, hook cracks, and selective seam weld corrosion — can fail along the seam and open a long split, which is why the historical record treats these lines as capable of larger releases than a pit in the body of the same pipe.
That description is the one PHMSA used in the January 2026 class-location preamble, 91 FR 1608, at the pages cited in Corrective Action Order CPF 4-2026-025-CAO. It is also the reason the 1998 hazardous-liquid rule on older pipe, 63 FR 59475, singled out pre-1970 ERW and lap-welded pipe susceptible to longitudinal seam failure as the population with the highest combination of failure probability and release volume.
Not the same seam as modern ERW
High-frequency ERW, the process used on most line pipe made since the early 1970s, is a different weld. The 15 January 2025 correction, after INGAA v. PHMSA, removed high-frequency ERW from the gas-transmission immediate-repair list for preferential metal loss. It did not remove low-frequency ERW, direct-current ERW, or electric-flash-welded seams. PHMSA’s July 2026 description of the gas criteria that remained still names preferential metal loss on DC-ERW, LF-ERW, electric-flash-welded pipe, or a joint with a factor below 1.0, at a failure-pressure ratio below 1.25, as an immediate condition. Read §192.714 and §192.933 before using that sentence as the list. The point that does not depend on the proposal is the one the correction already made: taking modern ERW off one immediate criterion was not a finding that vintage LF-ERW is ordinary pipe.
A joint factor below 1.0 in the design formula is the code’s older way of saying the seam is not entitled to the strength of the plate. Section 192.113 and the longitudinal-joint table are the gas text. A seam that was given a joint factor of 0.8 at design time is not analyzed, decades later, as if it were seamless.
What the assessment has to be able to do
For hazardous-liquid lines that could affect a high consequence area, §195.452(c)(1)(i) requires the integrity method chosen for low-frequency ERW pipe, or lap-welded pipe susceptible to longitudinal seam failure, to be capable of assessing seam integrity and of detecting corrosion and deformation anomalies. A metal-loss-only tool that is not capable of assessing the seam does not satisfy that sentence for this pipe, even when the same tool is an acceptable body-wall tool on seamless or high-frequency pipe.
Selective seam weld corrosion is the mechanism that makes the seam behave like a crack. The groove follows the bond line. A remaining-strength model written for blunt body-wall metal loss, including ordinary B31G, is the wrong model. Gas transmission puts crack-like defects, including this kind of seam, under §192.712(d): a fracture-mechanics analysis matched to the failure mode, and a fatigue analysis when the segment cycles. The crack note is the longer version. For liquid lines, FAQ 7.16 (12 September 2025) is the current PHMSA reading of corrosion “of or along” a longitudinal seam under §195.452(h): the 180-day criterion is for corrosive attack that specifically affects the seam, and isolated pits near a seam are not automatically in that bucket. The earlier interpretation, PI-17-0014, was withdrawn the same day.
Sleeves do not retire the seam
A steel sleeve over an LF-ERW seam does not determine whether the bond line is sound, and it can prevent the tool from seeing the seam it was supposed to assess. Magnetic flux leakage generally does not characterize metal loss under a steel shell. If the record of the sleeve does not say whether the seam was the defect being repaired, the operator has neither an assessment nor a description of the repair. That combination is what Corrective Action Order CPF 4-2026-025-CAO describes on the Marysville–Toledo crude line: 16-inch, 0.281-inch wall, X52, coal-tar coated, manufactured in 1967 with LF-ERW seams, and a release at a Type B sleeve whose original repair record could not be found. PHMSA’s order says the cause was still unknown when the order was issued. The pipe vintage is not offered there as the completed cause. It is offered as a known susceptibility on the segment that failed.
A Type A sleeve or a compression sleeve installed for some other defect on this pipe still leaves the seam in the carrier. Compression is a response to a longitudinal crack only when the crack, the fit, and the resulting stress state were actually established. It is not a seam-integrity assessment. A Type B sleeve can contain pressure if its own welds are sound. It does not erase a hook crack that is still in the bond line outside the sleeve, and the sleeve’s long seam is a weld of its own.
Cutting the joint out remains the repair that removes the seam. Grinding a seam defect is a repair only when the imperfection is gone and the remaining wall is still adequate, which is a high bar on a low-toughness bond line. Covering the seam and filing the location as repaired, without a record of what was covered, is the gap the repair-record rules already forbid. Those rules are in the repair records note.
Sources
- Pipeline Safety: Class Location Change Requirements, 91 FR 1608 — Federal Register
- Risk-Based Alternative to Pressure Testing Older Hazardous Liquid and Carbon Dioxide Pipelines, 63 FR 59475 — Federal Register
- 49 CFR 195.452 — eCFR
- 49 CFR 192.712 — eCFR
- 2025 corrections after INGAA v. PHMSA — Federal Register
- Corrective Action Order CPF 4-2026-025-CAO (PDF) — PHMSA
- Hazardous liquid integrity management FAQs, 12 September 2025 revision (FAQ 7.16) — PHMSA
Related notes
- Part 192 repair and integrity duties — Regulations and official guidance
- Part 195 repair and integrity duties — Regulations and official guidance
- Type B steel sleeves — Repair methods
- API RP 1160 — Codes and standards
Also in Defect assessment