06 · Coatings and corrosion protection

Field joint coatings

In short The plant coat stops at the weld. What gets applied in the field, and why that strip dominates coating failures.

Updated . Sources are listed at the end. Markdown version.

Plant coatings are applied to bare pipe before the bevels are welded. The girth weld, and a cutback on either side, is coated later, in the weather, on a schedule set by the firing line or by a bell hole. That strip is where holidays concentrate. It is also every place a cut-out adds two new welds. Section 192.461 applies to the field coating the same way it applies to the plant coating: it has to be applied on a prepared surface, it has to be compatible with cathodic protection, and it has to be inspected for holidays before the pipe is lowered in or backfilled.

The systems in common use are liquid epoxy, a heat-shrink sleeve over an epoxy primer, injection-molded polyethylene or polypropylene on a three-layer line, and — still, on older work — tape. They are not interchangeable across plant coatings. A heat-shrink sleeve that is correct on FBE can be the wrong stiffness and the wrong primer on 3LPE. A tape wrap used because it is fast recreates the shielding geometry the Marshall report and ADB-2016-04 exist to warn about, especially if the tape bridges a weld cap and leaves a tunnel.

Where field joints actually fail

The failures are repetitive, and they are not mysteries of resin chemistry:

  • The cutback was not blasted. The plant coat was feathered with a disk, the weld was wire-brushed, and the specification said near-white metal.
  • Condensation formed on a pipe that was below the dew point. The epoxy went on anyway.
  • The heat-shrink sleeve was under-heated, so the adhesive never flowed, or over-heated, so the plant polyethylene melted back and left a ledge.
  • The overlap onto the plant coat is too short, or the plant coat edge was left as a thick step that the field coat could not cover without a void.
  • The holiday detector voltage was wrong for the thickness, so either nothing was found or the detector burned new holes.

A repair dig has the same joint if the crew cut the pipe, and it has a cousin of the same joint wherever a sleeve or a grind meets old coating. Feather the old coat, prepare the steel to the grade the new material was qualified for, coat through the transition, and holiday-test the transition. Record the air temperature, the pipe temperature, the product, and the result. Those four lines are what a later corrosion dig will wish someone had written.

Compatibility with cathodic protection is a materials question, not a slogan. A field joint that shields — a disbondable polyolefin sleeve with no path for current, a tape tent — will look coated and will corrode. A field joint that holidays honestly will at least let the rectifier do the job Appendix D describes. Given the choice, honest holidays and a working cathodic-protection system beat a pretty shield.

Sources

  1. 49 CFR 192.461 — eCFR
  2. ADB-2016-04 — Federal Register
  3. NTSB/PAR-12/01 — NTSB
  4. AMPP — AMPP

Also in Coatings and corrosion protection

Spotted an error? Engineers keep this site honest.Report an error or suggest a correction