01 · Repair methods
Repairing girth welds and wrinkle bends
In short Girth welds and wrinkle bends fail under axial and bending load, not hoop stress. What §192.715 allows for a defective weld in service, why a hoop-only repair does not reinforce them, and what PHMSA's girth-weld advisory asked operators to review.
Most repair methods are designed around hoop stress, because corrosion and dents in the pipe body are governed by pressure acting around the circumference. A girth weld or a wrinkle bend is different. A circumferential flaw is opened by axial stress, which comes from bending, ground movement, thermal expansion, poor support, and the end-cap pressure load. A repair that adds only hoop strength does little for it.
Defective girth welds found in service
Section 192.715 covers gas transmission welds found unacceptable under the acceptance standards in §192.241(c), which point to API Std 1104 section 9 or Appendix A. Appendix A may not be used to accept cracks. The repair options are in order:
- Out of service. If the segment can be taken out of service, repair the weld under §192.245. That section requires removal, not repair, of a weld with a crack longer than 8% of the weld length (except offshore lay-vessel welds). Defects are removed to sound metal, the area is preheated if conditions call for it, and the repair is inspected. Crack repairs and repairs in a previously repaired area need a written repair procedure qualified under §192.225 that meets the original procedure’s minimum mechanical properties.
- In service by weld repair. Allowed under §192.715(b) only if all three conditions hold: the weld is not leaking; pressure is reduced so hoop stress is no more than 20% of SMYS; and grinding can be limited so at least 1/8 inch (3.2 mm) of weld thickness remains.
- Otherwise, a sleeve. A defective weld that cannot be repaired under the first two routes must be repaired by a full-encirclement welded split sleeve “of appropriate design.”
Section 192.719 requires each weld repair made under §§192.713, 192.715, and 192.717 to be examined under §192.241.
For hazardous liquid lines, §195.230 has the same remove-or-repair structure, the same 8% crack-length removal rule, and the same requirement for a procedure qualified under §195.214 for crack repairs. It sits in the construction subpart. Part 195 has no in-service weld repair section matching §192.715, so in-service work also relies on §195.422 and, in HCAs, §195.452(h).
What “appropriate design” means for a girth weld
A full-encirclement sleeve over a girth weld has to address the axial load path:
- Type B sleeves, with ends fillet-welded to the carrier, can contain pressure and transfer axial load across the weld. The fillet welds are in-service welds on the carrier and need a qualified in-service procedure. See Type B sleeves and in-service welding.
- Type A sleeves, not welded to the carrier, reinforce in the hoop direction only. They do not transfer axial load across a circumferential flaw and do not contain a leak. PHMSA’s ADB-2026-02 documents failures under Type A sleeves from water in the annulus, shielding, and fatigue at the unwelded ends. See Type A sleeves.
- Sleeves over a weld cap need a design that clears the reinforcement, such as a raised center section or filler in the annulus. Public examples on this site include a double-hump sleeve over a girth weld and epoxy-filled sleeves.
- Composite systems can reinforce girth welds only if the laminate includes axial fibers and the system has been tested for that use. The BSEE and PHMSA guideline says repairs of features other than corrosion, including girth welds, should be backed by full-scale destructive testing that includes axial and bending loads where they act. See Composite system types.
A cut-out removes the weld and the question. See Cut-out and replacement.
Dents and metal loss at girth welds
The repair criteria treat a weld as a stress concentrator. A dent deeper than 2% of diameter (0.250 inch below NPS 12) affecting curvature at a girth weld is a timed condition under §192.714, §192.933, and §195.452(h). Metal loss that could affect a girth weld is also on the timed lists, at a predicted-failure-pressure threshold in gas and at 50% predicted depth in liquid. See Repair schedules.
What the girth-weld advisory found
PHMSA’s ADB-10-03 (March 2010) followed hydrostatic test failures, in-service leaks, and failures of girth welds on several large-diameter (20-inch and larger), X70 and X80 pipelines built in 2008 and 2009. Post-incident testing found weld misalignment, improper bevels at wall-thickness transitions, improper back welds, and inadequate support of pipe and appurtenances. Some pipe ends did not meet diameter and out-of-roundness tolerances. Some NDT procedures were not optimized for the large wall-thickness variations at transitions. Many problem welds were in hilly terrain, at crossings and streams, and on slopes with unstable soil, where high stress concentration at the transition combined with poor support, poor backfill, and soil movement.
The advisory asked operators of those lines to review material specifications, field construction procedures, caliper and deformation tool results, welding procedures including back welding, NDT records, and any test or in-service failures. The lesson carries to repairs: a girth weld failure is often a load problem as much as a weld problem. A repair that does not address the support, the soil, or the bending that loaded the weld may see the same load again.
Wrinkle bends
A wrinkle bend is a field bend with deliberate folds on the inside of the bend, common in older construction. Section 192.315 prohibits making a wrinkle bend on gas pipe to be operated at 30% of SMYS or more, and sets limits for those that are made (no sharp kinks, wrinkles at least one diameter apart along the crotch, a deflection limit per wrinkle on pipe 16 inches and larger, and the long seam near the neutral axis). Section 195.212 prohibits wrinkle bends in liquid pipe outright. Lines built before these rules may still contain them.
A wrinkle is a local geometric strain concentration. It is most sensitive to bending and axial loads and to pressure cycling. The engineering questions for a wrinkle found by ILI or in a dig are the same as for a dent: the strain, the presence of cracking at the crest, the loads, and the cycles. Repair options are limited by geometry. A standard sleeve does not fit a bend. A fitted or filled sleeve, a composite system qualified for bends with axial reinforcement, or replacement with a modern bend are the usual choices. The composite guideline discusses wrinkle bends with the other non-corrosion features, and its recommendation for full-scale destructive testing of non-corrosion repairs applies to them.
Sources
- 49 CFR 192.715, transmission lines: permanent field repair of welds — eCFR
- 49 CFR 192.245, repair or removal of weld defects — eCFR
- 49 CFR 192.241, inspection and test of welds — eCFR
- 49 CFR 192.719, testing of repairs — eCFR
- 49 CFR 195.230, repair or removal of weld defects — eCFR
- 49 CFR 192.315, wrinkle bends in steel pipe — eCFR
- 49 CFR 195.212, bending of pipe — eCFR
- ADB-10-03, Girth Weld Quality Issues Due to Improper Transitioning, Misalignment, and Welding Practices of Large Diameter Line Pipe, 75 FR 14243 — Federal Register
- ADB-2026-02, integrity risks of Type A repair sleeves, 91 FR 3780 — Federal Register
- BSEE and PHMSA composite repair guideline (girth welds, wrinkle bends, branches) — BSEE
Related notes
- Advisory bulletins that bear on repair — Regulations and official guidance
- Repair schedules: gas transmission versus hazardous liquid — Regulations and official guidance
- Dents — Defect assessment
- Double-hump girth-weld sleeve on a 26-inch Kentucky gas line — Case studies
- Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe — Case studies
- ASME B31.8 and B31.8S — Codes and standards
Also in Repair methods
- Choosing a repair
- Composite wraps
- Type A steel sleeves
- Type B steel sleeves
- Mechanical and bolt-on clamps
- Cut-out and replacement
- Hot tapping and line plugging
- Grinding and recoat
- Hot taps: the regulatory prerequisites
- Epoxy-filled sleeves
- Steel compression sleeves
- Compression sleeves: questions engineers ask
- In-service welding and hydrogen pipelines
- Composite system types: pre-cured coil, wet lay-up, and pre-preg
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction