07 · Case studies
Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe
In short MFL-visible composite reinforcement of an internal weld defect on a 24-inch refined-products line cured at -7 C with heating blankets.
Source: WrapMaster / Tecma (vendor case-study PDF). Account type: Vendor account.
In-line inspection of a 24-inch Western European refined-products line (67 bar design) found a 12-by-15 mm internal weld defect, 5.1 mm deep. The regulator required reinforcement. The operator lowered pressure to 24 bar but kept the line full while trained technicians blasted the surface, applied epoxy, and installed a composite weld-wrap sleeve, which includes a metallic mesh so MFL tools can see the repair. Because the air temperature was -7 C, a heating blanket was used; the vendor says installation took less than an hour and the wrap was cured in four hours. This is a manufacturer PDF, but it gives unusually complete defect and pressure data.
Method
WrapMaster Weld Wrap composite sleeve, designed to ISO 24817 and described as a permanent ASME B31.4 composite-sleeve repair, with a metallic mesh for MFL detectability
Defect
Internal weld defect, 12 by 15 mm, 5.1 mm deep, found by in-line inspection
Pipe
24-inch refined-products transmission pipeline, Western Europe, 67 bar gauge design pressure, 20 C operating temperature. Pressure was reduced to 24 bar gauge during installation and cure. Ambient temperature during installation was -7 C.
Outcome
The vendor reports the sleeve was installed in less than an hour, fully cured within four hours under a heating blanket, and that the line stayed full of product at reduced pressure. Acceptance as a permanent repair is stated by the manufacturer with reference to ASME B31.4 and ISO 24817.
Schedule, cost, and service-life figures in this note are the publisher’s claims. They were not checked against an operator record or a laboratory report.
Dates: Year not stated. PDF hosted by a 2024-dated path.
Maker named in the source: WrapMaster.
Sources
- WrapMaster Weld Wrap reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe — WrapMaster / Tecma (vendor case-study PDF)
Related notes
- Composite wraps — Repair methods
- ASME PCC-2 — Codes and standards
- ISO 24817 — Codes and standards
- Corrosion metal loss — Defect assessment
- AB-539: engineered composite alterations in Alberta — Regulations and official guidance
- Choosing a repair — Repair methods
Also in Case studies
- Type A sleeve leak on the Twin Oaks Pipeline, Upper Makefield Township, Pennsylvania
- Type B sleeve leak on the Marysville-Toledo Crude Pipeline, Sterling Heights, Michigan (CAO 4-2026-025)
- Type A sleeve leak on Colonial Line 1, Huntersville, North Carolina (CPF 2-2021-005-NOPSO)
- Type A sleeve leak on Colonial Line, Gwinnett County (Harbins Road), Georgia
- Type A sleeve leak on the CNG/Plantation pipeline, Belton, South Carolina
- Type C compression-sleeve repairs on the Oasis Pipeline, Texas
- In-service X70 Type B sleeve installation on West-East Gas Pipeline Line 3, China
- Subsea Clamp+Sleeve repair of a buckled 10-inch crude line, South Marsh Island Block 59
- ROV-installed Flange Repair Split+Sleeve on a 10-inch water-injection line, offshore Angola
- ROV-installed leak-sealing clamp on a 10-inch water-injection riser flange, Foinaven field
- Emergency leak repair on a 30-inch onshore pipeline with a bolt-on fitting
- Composite sleeve repair of 900 feet of cooling-tower corrosion on a U.S. refinery pipeline
- Composite sleeve repair of a dent and seam-weld crack on a 24-inch crude-oil pipeline
- Underwater composite sleeve repair of girth-weld corrosion on a 12-inch gas pipeline
- Composite sleeve repair of a rockfall dent on a 36-inch hydroelectric pipeline in the French Alps
- Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)
- Composite pipe-wrap repairs of corrosion on Equistar Pipeline, Texas
- Composite repair of a 32-inch offshore riser, Thailand
- Splash-zone composite repair of mechanical damage on a 12-inch subsea crude line, Gulf of Mexico
- Carbon-fiber repair of a deep crack on a 900 mm gas-transmission bend
- Epoxy-filled sleeve encapsulation of a large dent on a 14-inch trunkline, Papua New Guinea
- High-pressure line-plug isolation to remove a stuck pig and replace a leaking valve on a CO2 pipeline
- Line-plug train isolation and diversion of two 24-inch gas transmission lines under a planned Singapore subway station
- Line-plug train isolation to decommission a gas-processing plant off a 36-inch transmission line, Alabama
- Emergency double line-plug isolation of a burning 14-inch NGL pipeline after a third-party strike, West Texas
- 12-inch double line-plug isolation with bypass for a live gas-line repair, Oklahoma
- Line stop to connect 8-inch PE gas mains, St. Louis
- Insertion valves and line stops after a sheared 8-inch valve, Covington, Ohio
- Epoxy recoating of HDD-damaged girth and spiral welds, Kansas
- West Virginia 30-inch leak at a previous composite wrap
- Port Allen valve-station dent reinforced with an E-glass wrap
- 14-inch diesel line at Redding, Pennsylvania, carbon wrap
- Hinged protective tools on a 24-inch Florida line during bridge work
- Custom Type B sleeve around an existing clamp, Florida
- Type B sleeves replacing mechanical clamps at a Texas refinery
- Double-hump girth-weld sleeve on a 26-inch Kentucky gas line
- Compression sleeve on a crude line, Middle East operator
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction