09 · Test reports

Fatigue testing of composite repairs on dented pipe, 2010

In short Unrepaired 15 percent dents on 12.75-inch X42 pipe averaged 10,957 cycles at a 0-to-892 psi range. Two of eight composite systems reached a 250,000-cycle run-out with no failures in any of their repaired dents.

Updated . Sources are listed at the end. Markdown version.

Source: Alexander, C., and Bedoya, J. (Stress Engineering Services, Inc.). “Repair of Dents Subjected to Cyclic Pressure Service Using Composite Materials.” Proceedings of the 8th International Pipeline Conference, paper IPC2010-31524, Calgary, Alberta, 27 September–1 October 2010. ASME. DOI: 10.1115/IPC2010-31524.

What was tested

Eight composite repair systems, and an unrepaired control set, on plain dents, dents in girth welds, and dents in high-frequency ERW seams. The pipe was 12.75-inch outside diameter, 0.188-inch wall, Grade X42.

Setup

Six dents were installed in each sample with a 4-inch spherical end cap to an initial depth of 15 percent of outside diameter. The first dent was made, then the pipe was pressurized to 72 percent of SMYS (892 psi) with the indenter still in place; the remaining dents were also made with internal pressure. After all six dents were in, ten pressure cycles from 0 to 892 psi were applied and residual profiles were measured. Girth welds were X-rayed after denting. Each manufacturer designed its own repair, including length and thickness; measured repair thicknesses ranged from 0.175 inch to 0.671 inch. Filler was used in the dents. Samples were then cycled from 0 to 100 percent of MAOP (0 to 892 psi, with MAOP taken as 72 percent of SMYS) to failure or to a 250,000-cycle run-out. Failed dents were cut out so cycling of the remaining dents could continue. Strain gages were placed in the dented region.

Key numbers

The average cycles to failure for the six unrepaired dents was 10,957. The target for those unrepaired dents had been about 10,000 cycles.

Two of the eight systems — a carbon/epoxy system and a pre-cured E-glass system — reached 250,000 cycles with no failures in any of their repaired dents. A third system had an average life of 215,271 cycles. One system was later cycled beyond run-out; the ERW seam failed at 358,470 cycles.

Stress amplification factors calculated from the measured lives were highest for the unrepaired dents, with a maximum of 3.76 for an unrepaired dent in an ERW seam. The two systems that reached run-out had SAFs of 1.49. The paper reports no direct correlation between composite thickness and cycles to failure, and attributes part of the difference among systems to the load-transfer filler.

Takeaways

On this program, unrepaired 15 percent dents failed on the order of 10,000 cycles at a 72 percent SMYS pressure range, while two of the eight wraps reached the 250,000-cycle run-out on every dent type in the matrix. Thickness alone did not explain the ranking. The 250,000-cycle stop is a run-out, not a measured failure life, except for the one system later taken to an ERW-seam failure at 358,470 cycles.

The paper is available from ASME.

Sources

  1. Repair of Dents Subjected to Cyclic Pressure Service Using Composite Materials (IPC2010-31524) — ASME 8th International Pipeline Conference, 2010

Also in Test reports

Spotted an error? Engineers keep this site honest.Report an error or suggest a correction

Open the form on this page

Occasional updates