09 · Test reports
Long-term subsea exposure testing of composite repairs, 2017
In short Fifteen underwater-installed composite repairs on 12.75-inch X42 pipe with 75 percent corrosion all held 10,000 hours at 72 percent of SMYS in simulated seawater. After ultraviolet exposure, thermal cycling, and pressure cycling, burst pressures were 1,681 psi unrepaired, 4,037 psi for Manufacturer B, and 3,615 psi for Manufacturer C.
Source: Sheets, C., Futch, D., and Denowh, C.; reviewed by Vyvial, B. A. (Stress Engineering Services, Inc.). Results of the Long-Term Subsea 10,000hr Testing. Final report, SES Document No. 1461191-PL-RP-04, Rev 0, 2 November 2017. Prepared for the Bureau of Safety and Environmental Enforcement and the Pipeline and Hazardous Materials Safety Administration, Contract No. E15PC00003 / DTPH5615X00016 (PHMSA project 658).
What was tested
Three commercial composite repair systems, installed underwater, on 12.75-inch outside diameter, 0.375-inch wall, Grade X42 pipe with a 6-inch by 8-inch machined corrosion patch 75 percent of wall deep. Fifteen samples (five from each manufacturer) were held for 10,000 hours in simulated seawater and then put through ultraviolet exposure, thermal cycling, pressure cycling, burst, tension, and bending. Each manufacturer also provided a sample with an intentional installation defect, used to look at delamination.
Setup
The 10,000-hour hold was at 72 percent of SMYS, within plus or minus 15 percent, in water targeted at 32 parts per thousand salinity. After the hold, samples received 90 days of ultraviolet exposure and 12 thermal cycles with a range of about 100 °F and a maximum of about 130 °F. They were then pressure-cycled from 890 to 1,780 psi (36 to 72 percent of SMYS). The run-out target was 25,000 cycles for the tension and bending samples and 50,000 cycles for the others. Samples that completed that pre-cycling went on to burst, fatigue-to-failure, tension, or bending. Tension and bending were run with 1,780 psi internal pressure. Bending moments are reported for the orientation that put the corrosion in compression. The tension loads in the table below are the loads applied by the frame and do not include pressure end load (201.3 kips at 1,780 psi).
Key numbers
All 15 samples completed the 10,000-hour seawater hold without failure.
Pre-cycling after the ultraviolet and thermal exposure:
- Burst-designated samples: Manufacturer A failed after 17,411 cycles; Manufacturers B and C survived.
- Fatigue-designated samples: Manufacturer A failed after 31,547 cycles; B and C survived.
- Tension-designated samples: Manufacturer A failed after 3,678 cycles; B and C survived.
- Bending-designated samples: all three manufacturers survived.
- Intentional-delamination samples: Manufacturer A failed after 23,237 cycles; B after 42,223 cycles; C survived.
Burst, after that exposure sequence. Unrepaired: 1,681 psi, in the simulated corrosion. Manufacturer A had no burst pressure (the burst-designated sample had already failed in pre-cycling). Manufacturer B: 4,037 psi, in the base pipe outside the repair. Manufacturer C: 3,615 psi, in the simulated corrosion under the repair. Both reported repairs were at least twice the unrepaired burst pressure.
Further pressure cycling after the 50,000-cycle pre-cycle (cycle counts include those pre-cycles): Manufacturer B failed at 130,960 cycles; Manufacturer C reached the 250,000-cycle run-out (50,000 pre-cycles plus 200,000 more) without failure. An unrepaired sample did not complete one cycle to 1,780 psi. Manufacturer A’s fatigue life is the 31,547 cycles already recorded in pre-cycling.
Tension to failure (frame load only): Manufacturer B 604.7 kips; Manufacturer C 620.0 kips; Manufacturer C delamination sample 635.0 kips. All three failed in the simulated corrosion under the repair, and all three exceeded 600 kips.
Bending to failure, with 1,780 psi held: Manufacturer A 264.6 kip-feet; Manufacturer B 262.4 kip-feet; Manufacturer C 278.4 kip-feet. All three exceeded 260 kip-feet.
Takeaways
The 10,000-hour hold itself produced no failures. After ultraviolet exposure, thermal cycling, and pressure cycling, the two repairs that were burst failed at more than twice the unrepaired burst pressure; one failed in the carrier pipe outside the wrap and one in the corrosion under the wrap. Fatigue lives after that same exposure sequence ranged from a pre-cycle failure at 17,411 cycles on a Manufacturer A burst sample to a 250,000-cycle run-out on Manufacturer C. The report is limited to external corrosion of this geometry and says further work would be needed before using the systems on other anomaly types, including planar flaws.
Download the report. The project record is on PHMSA PRIMIS (project 658), and BSEE also posts the file at 763ACv1.pdf.
Sources
- Results of the Long-Term Subsea 10,000hr Testing, Final Report (1461191-PL-RP-04, Rev 0) — BSEE / PHMSA / Stress Engineering Services, November 2017
- PHMSA project 658 — Pipeline and Hazardous Materials Safety Administration
Related notes
- Type B steel sleeves — Repair methods
- Steel compression sleeves — Repair methods
- Dents — Defect assessment
- Steel repair sleeve MAOP tables — Assessment
- Test reports and downloads — Test reports
Also in Test reports
- Burst test of a 24-inch leaking pipe with a Type B sleeve, 2019
- Type B sleeve fit-up, tight and loose, 2021
- Backing-strip mill groove on a Type B sleeve, 2021
- Full-scale testing of a compression sleeve, 2022
- Manual pipe-jack torque test, 2019
- Steel sleeves reinforcing corrosion and plain dents, 2021
- Composite repairs of corroded riser pipe under pressure, tension, and bending, 2007
- Repair of dent-and-gouge damage by grinding and composite wraps, 2009
- Fatigue testing of composite repairs on dented pipe, 2010
- Fatigue and burst testing of composite and steel-sleeve repairs on corrosion and dents, 2014
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction