07 · Case studies
Composite sleeve repair of a dent and seam-weld crack on a 24-inch crude-oil pipeline
In short Non-welded pre-cured composite reinforcement of a dent and ground-out seam-weld crack on a 24-inch X52 crude pipeline.
Source: CSNRI / Critica Infrastructure (Clock Spring). Account type: Vendor account.
An onshore 24-inch X52 crude line had a dent and a crack in a seam weld. The operator wanted to avoid welding and had already looked at a carbon-fiber wrap, which it considered too slow and costly. The line was taken out of service but left full while technicians ground out the crack, filled the dent, and installed two pre-cured composite sleeves by hand spool. CSNRI says two local technicians finished the installation in about four hours. As with other manufacturer case studies, the performance and cost comparisons should be read as the vendor’s claims.
Method
Crack ground out, dent filled, then two standard 24-inch Clock Spring composite sleeves installed by the hand-spool method, plus a single-wrap mold and two filler kits
Defect
Dent with a crack in the seam weld
Pipe
24-inch (610 mm) carbon steel API X52 crude-oil pipeline, onshore (technicians described as coming from the Netherlands). Operating pressure not stated. The line was taken out of service but not evacuated during grinding.
Outcome
CSNRI reports two technicians finished the sleeves in about four hours, with no welding, and describes the work as about 25 percent of the time and 35 percent of the cost of an alternative (unspecified) solution, with a 50-year validated service life. Time, cost, and life claims are the vendor’s.
Schedule, cost, and service-life figures in this note are the publisher’s claims. They were not checked against an operator record or a laboratory report.
Dates: Year not stated.
Maker named in the source: CSNRI (Clock Spring).
Sources
- Clock Spring repair of a dent and seam-weld crack on a 24-inch crude-oil pipeline — CSNRI / Critica Infrastructure (Clock Spring)
Related notes
- Composite wraps — Repair methods
- ASME PCC-2 — Codes and standards
- ISO 24817 — Codes and standards
- Corrosion metal loss — Defect assessment
- AB-539: engineered composite alterations in Alberta — Regulations and official guidance
- Choosing a repair — Repair methods
Also in Case studies
- Type A sleeve leak on the Twin Oaks Pipeline, Upper Makefield Township, Pennsylvania
- Type B sleeve leak on the Marysville-Toledo Crude Pipeline, Sterling Heights, Michigan (CAO 4-2026-025)
- Type A sleeve leak on Colonial Line 1, Huntersville, North Carolina (CPF 2-2021-005-NOPSO)
- Type A sleeve leak on Colonial Line, Gwinnett County (Harbins Road), Georgia
- Type A sleeve leak on the CNG/Plantation pipeline, Belton, South Carolina
- Type C compression-sleeve repairs on the Oasis Pipeline, Texas
- In-service X70 Type B sleeve installation on West-East Gas Pipeline Line 3, China
- Subsea Clamp+Sleeve repair of a buckled 10-inch crude line, South Marsh Island Block 59
- ROV-installed Flange Repair Split+Sleeve on a 10-inch water-injection line, offshore Angola
- ROV-installed leak-sealing clamp on a 10-inch water-injection riser flange, Foinaven field
- Emergency leak repair on a 30-inch onshore pipeline with a bolt-on fitting
- Composite sleeve repair of 900 feet of cooling-tower corrosion on a U.S. refinery pipeline
- Underwater composite sleeve repair of girth-weld corrosion on a 12-inch gas pipeline
- Composite sleeve repair of a rockfall dent on a 36-inch hydroelectric pipeline in the French Alps
- Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)
- Composite pipe-wrap repairs of corrosion on Equistar Pipeline, Texas
- Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe
- Composite repair of a 32-inch offshore riser, Thailand
- Splash-zone composite repair of mechanical damage on a 12-inch subsea crude line, Gulf of Mexico
- Carbon-fiber repair of a deep crack on a 900 mm gas-transmission bend
- Epoxy-filled sleeve encapsulation of a large dent on a 14-inch trunkline, Papua New Guinea
- High-pressure line-plug isolation to remove a stuck pig and replace a leaking valve on a CO2 pipeline
- Line-plug train isolation and diversion of two 24-inch gas transmission lines under a planned Singapore subway station
- Line-plug train isolation to decommission a gas-processing plant off a 36-inch transmission line, Alabama
- Emergency double line-plug isolation of a burning 14-inch NGL pipeline after a third-party strike, West Texas
- 12-inch double line-plug isolation with bypass for a live gas-line repair, Oklahoma
- Line stop to connect 8-inch PE gas mains, St. Louis
- Insertion valves and line stops after a sheared 8-inch valve, Covington, Ohio
- Epoxy recoating of HDD-damaged girth and spiral welds, Kansas
- West Virginia 30-inch leak at a previous composite wrap
- Port Allen valve-station dent reinforced with an E-glass wrap
- 14-inch diesel line at Redding, Pennsylvania, carbon wrap
- Hinged protective tools on a 24-inch Florida line during bridge work
- Custom Type B sleeve around an existing clamp, Florida
- Type B sleeves replacing mechanical clamps at a Texas refinery
- Double-hump girth-weld sleeve on a 26-inch Kentucky gas line
- Compression sleeve on a crude line, Middle East operator
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction