07 · Case studies
Compression sleeve on a crude line, Middle East operator
In short A shop trial and a first live compression-sleeve install, taken from a forthcoming conference paper. The operator is not named because the paper is not in the public proceedings.
Source: forthcoming conference paper (2026). The draft is not hosted. A search of the public IPC 2026 proceedings on 25 November 2026 did not find this paper listed, so the operator is described as a Middle East operator and the citation stays forthcoming.
The paper describes two steps.
In a September 2025 shop trial, a fabricated 24-inch, Grade X60, 0.5-inch wall joint carried an artificial crack 6 inches long and 50 percent deep. A compression sleeve was dry-fitted, heated to about 400°F (204°C) in about four minutes, tacked, and welded on the long seams. The spool was then pressure-cycled between 36 and 72 percent of SMYS for 10 cycles. After the sleeve was cut off, shear-wave ultrasonic testing and pit-gauge readings showed no crack growth. The draft abstract also describes cyclic testing near 1,800 psi with no leak. The body figures — 36 to 72 percent of SMYS, 10 cycles, no growth — are the ones used here.
On the live line, an ultrasonic crack-detection inspection found a 47 percent deep crack in a seam weld. The compression sleeve on hand was sized for 30-inch pipe and the defect was on a 31-inch section, so the crew shortened the circumference of a conventional 31-inch steel sleeve and dry-fitted it three times. The line was not shut down, and a cut-out was avoided. Crack-growth checks are planned on the next in-line inspection, so the field result is not yet reported.
Figures in the draft, reported here as draft calculations rather than a third-party audit: pipe 31-inch outside diameter by 0.251-inch wall, specified minimum yield strength 52 ksi; sleeve 32.25-inch outside diameter by 0.625-inch wall, specified minimum yield strength 65 ksi; induction target 400°F; line pressure during installation 80 psi; calculated interface pressure about 99 psi after heating, cooling, and internal pressure. The paper’s wording “API PCC-2” is treated as a slip for ASME PCC-2.
Sources
Related notes
- Steel compression sleeves — Repair methods
- Compression sleeves: questions engineers ask — Repair methods
- Full-scale testing of a compression sleeve, 2022 — Test reports
- ASME PCC-2 — Codes and standards
- Part 192 repair and integrity duties — Regulations and official guidance
- Choosing a repair — Repair methods
Also in Case studies
- Type A sleeve leak on the Twin Oaks Pipeline, Upper Makefield Township, Pennsylvania
- Type B sleeve leak on the Marysville-Toledo Crude Pipeline, Sterling Heights, Michigan (CAO 4-2026-025)
- Type A sleeve leak on Colonial Line 1, Huntersville, North Carolina (CPF 2-2021-005-NOPSO)
- Type A sleeve leak on Colonial Line, Gwinnett County (Harbins Road), Georgia
- Type A sleeve leak on the CNG/Plantation pipeline, Belton, South Carolina
- Type C compression-sleeve repairs on the Oasis Pipeline, Texas
- In-service X70 Type B sleeve installation on West-East Gas Pipeline Line 3, China
- Subsea Clamp+Sleeve repair of a buckled 10-inch crude line, South Marsh Island Block 59
- ROV-installed Flange Repair Split+Sleeve on a 10-inch water-injection line, offshore Angola
- ROV-installed leak-sealing clamp on a 10-inch water-injection riser flange, Foinaven field
- Emergency leak repair on a 30-inch onshore pipeline with a bolt-on fitting
- Composite sleeve repair of 900 feet of cooling-tower corrosion on a U.S. refinery pipeline
- Composite sleeve repair of a dent and seam-weld crack on a 24-inch crude-oil pipeline
- Underwater composite sleeve repair of girth-weld corrosion on a 12-inch gas pipeline
- Composite sleeve repair of a rockfall dent on a 36-inch hydroelectric pipeline in the French Alps
- Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)
- Composite pipe-wrap repairs of corrosion on Equistar Pipeline, Texas
- Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe
- Composite repair of a 32-inch offshore riser, Thailand
- Splash-zone composite repair of mechanical damage on a 12-inch subsea crude line, Gulf of Mexico
- Carbon-fiber repair of a deep crack on a 900 mm gas-transmission bend
- Epoxy-filled sleeve encapsulation of a large dent on a 14-inch trunkline, Papua New Guinea
- High-pressure line-plug isolation to remove a stuck pig and replace a leaking valve on a CO2 pipeline
- Line-plug train isolation and diversion of two 24-inch gas transmission lines under a planned Singapore subway station
- Line-plug train isolation to decommission a gas-processing plant off a 36-inch transmission line, Alabama
- Emergency double line-plug isolation of a burning 14-inch NGL pipeline after a third-party strike, West Texas
- 12-inch double line-plug isolation with bypass for a live gas-line repair, Oklahoma
- Line stop to connect 8-inch PE gas mains, St. Louis
- Insertion valves and line stops after a sheared 8-inch valve, Covington, Ohio
- Epoxy recoating of HDD-damaged girth and spiral welds, Kansas
- West Virginia 30-inch leak at a previous composite wrap
- Port Allen valve-station dent reinforced with an E-glass wrap
- 14-inch diesel line at Redding, Pennsylvania, carbon wrap
- Hinged protective tools on a 24-inch Florida line during bridge work
- Custom Type B sleeve around an existing clamp, Florida
- Type B sleeves replacing mechanical clamps at a Texas refinery
- Double-hump girth-weld sleeve on a 26-inch Kentucky gas line
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction