07 · Case studies
Burst test of a composite sleeve repair recovered after 25 years in service (installed 1995)
In short Hydrostatic burst test of a pre-cured composite sleeve cut out after 25 years in gas service; pipe ruptured at 2,180 psi outside the repair.
Source: CSNRI, in World Pipelines (April 2021), describing a test on pipe removed by the operator (2020). Account type: Vendor field test.
In 1995 an operator repaired a 12-inch-long, 63-percent corrosion defect on a gas line (750 psi operating, 970 psi MAOP) with a pre-cured composite sleeve while the line stayed in service. At the end of 2020 that pipe section was cut out during other work and offered to CSNRI for testing. The repaired joint held 1,455 psi for five minutes and later burst at 2,180 psi, with the rupture in unrepaired pipe, not under the sleeve. Tensile tests on the old composite were reported at 90,000 psi. Because opportunities to test 25-year-old field repairs are rare, this is one of the more useful public composite data points, even though the write-up is by the manufacturer.
Method
Clock Spring composite repair sleeve, originally installed in service over filler in corroded areas
Defect
External corrosion, multiple defects; the worst was 12 inches long with 63 percent wall loss
Pipe
Carbon-steel natural-gas pipeline operating at 750 psi, MAOP 970 psi, at the time of the 1995 repair. Diameter is not stated in the article.
Outcome
The recovered, repaired joint was held at 1,455 psi (1.5 times MAOP) for five minutes, then taken to burst. It ruptured at 2,180 psi in pipe outside the repaired area. Coupon tensile tests on the 25-year-old composite were reported at 90,000 psi, which the authors say showed no meaningful degradation. The article is written by CSNRI, but it reports a full-scale test on a real field repair removed by the operator.
Schedule, cost, and service-life figures in this note are the publisher’s claims. They were not checked against an operator record or a laboratory report.
Dates: Repair installed in 1995. Pipe section removed and tested at the end of 2020. Article reprinted April 2021.
Maker named in the source: CSNRI (Clock Spring).
Sources
- Burst test of a Clock Spring repair recovered after 25 years in service (installed 1995) — CSNRI, in World Pipelines (April 2021), describing a test on pipe removed by the operator
Related notes
- Composite wraps — Repair methods
- ASME PCC-2 — Codes and standards
- ISO 24817 — Codes and standards
- Corrosion metal loss — Defect assessment
- AB-539: engineered composite alterations in Alberta — Regulations and official guidance
- Choosing a repair — Repair methods
Also in Case studies
- Type A sleeve leak on the Twin Oaks Pipeline, Upper Makefield Township, Pennsylvania
- Type B sleeve leak on the Marysville-Toledo Crude Pipeline, Sterling Heights, Michigan (CAO 4-2026-025)
- Type A sleeve leak on Colonial Line 1, Huntersville, North Carolina (CPF 2-2021-005-NOPSO)
- Type A sleeve leak on Colonial Line, Gwinnett County (Harbins Road), Georgia
- Type A sleeve leak on the CNG/Plantation pipeline, Belton, South Carolina
- Type C compression-sleeve repairs on the Oasis Pipeline, Texas
- In-service X70 Type B sleeve installation on West-East Gas Pipeline Line 3, China
- Subsea Clamp+Sleeve repair of a buckled 10-inch crude line, South Marsh Island Block 59
- ROV-installed Flange Repair Split+Sleeve on a 10-inch water-injection line, offshore Angola
- ROV-installed leak-sealing clamp on a 10-inch water-injection riser flange, Foinaven field
- Emergency leak repair on a 30-inch onshore pipeline with a bolt-on fitting
- Composite sleeve repair of 900 feet of cooling-tower corrosion on a U.S. refinery pipeline
- Composite sleeve repair of a dent and seam-weld crack on a 24-inch crude-oil pipeline
- Underwater composite sleeve repair of girth-weld corrosion on a 12-inch gas pipeline
- Composite sleeve repair of a rockfall dent on a 36-inch hydroelectric pipeline in the French Alps
- Composite pipe-wrap repairs of corrosion on Equistar Pipeline, Texas
- Weld-wrap composite reinforcement of an internal weld defect on a 24-inch products pipeline, Western Europe
- Composite repair of a 32-inch offshore riser, Thailand
- Splash-zone composite repair of mechanical damage on a 12-inch subsea crude line, Gulf of Mexico
- Carbon-fiber repair of a deep crack on a 900 mm gas-transmission bend
- Epoxy-filled sleeve encapsulation of a large dent on a 14-inch trunkline, Papua New Guinea
- High-pressure line-plug isolation to remove a stuck pig and replace a leaking valve on a CO2 pipeline
- Line-plug train isolation and diversion of two 24-inch gas transmission lines under a planned Singapore subway station
- Line-plug train isolation to decommission a gas-processing plant off a 36-inch transmission line, Alabama
- Emergency double line-plug isolation of a burning 14-inch NGL pipeline after a third-party strike, West Texas
- 12-inch double line-plug isolation with bypass for a live gas-line repair, Oklahoma
- Line stop to connect 8-inch PE gas mains, St. Louis
- Insertion valves and line stops after a sheared 8-inch valve, Covington, Ohio
- Epoxy recoating of HDD-damaged girth and spiral welds, Kansas
- West Virginia 30-inch leak at a previous composite wrap
- Port Allen valve-station dent reinforced with an E-glass wrap
- 14-inch diesel line at Redding, Pennsylvania, carbon wrap
- Hinged protective tools on a 24-inch Florida line during bridge work
- Custom Type B sleeve around an existing clamp, Florida
- Type B sleeves replacing mechanical clamps at a Texas refinery
- Double-hump girth-weld sleeve on a 26-inch Kentucky gas line
- Compression sleeve on a crude line, Middle East operator
Spotted an error? Engineers keep this site honest.Report an error or suggest a correction